Skip to content

Cleaning and Corrosion Control

What corrosion needs in order to happen, the types and where they hide, removal and treatment, and the finishing that keeps it out.

Everything here follows from four conditions that must exist together: an anode, a cathode, a conductive path and an electrolyte. Remove any one and corrosion stops, which is why paint is a corrosion control measure rather than decoration.

The types are worth separating by what they look like and where they are found. Surface corrosion is a white powder on aluminium and red rust on steel. Intergranular runs along grain boundaries with little to see outside. Exfoliation lifts rolled metal into layers like a wet book. Filiform crawls under a coating in fine threads. Galvanic happens where two dissimilar metals meet with an electrolyte present.

Treatment order never changes. Remove all the corrosion products down to sound metal first, then treat, then refinish. Anything left under the new coating carries on working where nobody can see it.

The one absolute prohibition is steel wool or a steel brush on aluminium. Embedded steel particles create fresh galvanic cells, so the treatment causes the disease.

Electrolyte: the conductive liquid, usually water carrying salts, that lets the corrosion cell work.

Conversion coating: a chemical film on aluminium that resists corrosion and helps paint adhere.

Anodising: an electrolytic process thickening the natural oxide layer. It cannot be restored in the field.

Corrosion preventive compound: a film that displaces moisture, applied after cleaning and renewed on a schedule.

Exfoliation: intergranular attack that delaminates rolled or extruded metal into visible layers.

When a question names two different metals in contact it is asking about galvanic corrosion, and the answer involves a barrier between them.

Control surfaces are rebalanced after refinishing. Flutter develops in seconds and the balance limits are not advisory, so any answer suggesting the paint weight does not matter is wrong.

Registration marks and required placards go back on after painting. An aircraft without them is not airworthy, whatever else is right.